Content page
From [Institution name]
| Property |
Requirement |
Result |
|---|---|---|
| Thickness (mm) |
≥ 0.33 |
0.42 |
| Thickness of aluminum-zinc coating (g/m2) |
≥ 150 |
171 |
| Flexibility |
No flaking or micro-cracking |
Pass |
| Humidity resistance |
No formation of blisters |
Pass |
| Salt spray resistance |
≥ 7 rating |
Pass |
| Durability |
Slight colour change; not greater than No. 8 degree of chalking; no flaking or cracking |
Pass |
| Pressure (kPa) |
Time (min) |
Requirement |
Result |
|---|---|---|---|
0.8 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
1.2 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
1.5 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
1.9 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
2.7 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
5.8 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
6.5 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
7.2 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
7.9 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
8.6Footnote (2) |
1 |
– |
Fasteners pulled through battens |
| Pressure (kPa) |
Time (min) |
Requirement |
Result |
|---|---|---|---|
| 0.8 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
| 1.2 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
| 1.5 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
| 1.9 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
| 2.7 |
5 |
No evidence of deformation, permanent damage or failure |
Pass |
| 5.8 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 6.5 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 7.2 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 7.9 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 8.6 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 9.4 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 10.1 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 10.8 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 11.5 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 12.2 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 13.0 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 13.7 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 14.4 |
1 |
No evidence of deformation, permanent damage or failure |
Pass |
| 15.1Footnote (2) |
1 |
– |
Fasteners pulled through battens |
| Wind SpeedFootnote (2) (km/h) |
Simulated Rainfall (L/m2·min) |
Duration (min) |
Requirement |
Result |
|---|---|---|---|---|
50 |
3.7 |
15 |
No leakage or damage |
Pass |
110 |
3.7 |
15 |
No leakage or damage |
Pass |
140 |
3.7 |
15 |
No leakage or damage |
Pass |
170 |
3.7 |
5 |
No leakage or damage |
Pass |