Content page
From [Institution name]
RSI (m2·K/W) |
Cavity Depth (mm) |
Applied Density (kg/m3) |
Bag Usage (Bags/100 m2) |
Maximum Coverage (m2/Bag) |
---|---|---|---|---|
2.5 |
89 |
24.0 |
14.7 |
6.8 |
3.9 |
140 |
24.0 |
23.2 |
4.3 |
5.1 |
184 |
24.0 |
30.5 |
3.3 |
6.5 |
235 |
24.0 |
38.9 |
2.6 |
2.7 |
89 |
30.4 |
18.7 |
5.4 |
4.1 |
140 |
30.4 |
29.4 |
3.4 |
5.5 |
184 |
30.4 |
38.6 |
2.6 |
7.0 |
235 |
30.4 |
49.3 |
2.0 |
Specimen |
Moisture Content (%) |
Density (kg/m3) |
---|---|---|
A |
15.2 |
31.56 |
B |
19.0 |
34.14 |
C |
12.5 |
30.75 |
Average |
15.6 |
32.15 |
Specimen |
Specimen Density (kg/m3) |
Corresponding Thermal Resistance (m2·K/W) |
---|---|---|
A |
30.56 |
4.27 |
B |
31.00 |
4.31 |
C |
30.86 |
4.36 |
Average |
30.81 |
4.31 |
Property |
Result |
---|---|
Smoulder resistance |
No evidence of flaming combustion during the tests |
Flame-spread classification (FSC) |
5 |
Smoke-developed classification (SDC) |
5 |